All of the electrodes listed below should be stored dry at room temp when in unopened cartons.

Electrode Classification
Recommended Storage open Boxes
Holding Oven
Reconditioning
E-XX10
Dry @ room temp
Not Recommended
Not done
E-XX11
Dry @ room temp
Not Recommended
Not done
E-XX12
Dry @ room temp
Not Recommended
Not done
E-XX13
Dry @ room temp
Not Recommended
Not done
E-XX14
150 - 200 F
150 - 200 F
250 - 300 F 1 hr.
E-XX20
150 - 200 F
150 - 200 F
250 - 300 F 1 hr.
E-XX24
150 - 200 F
150 - 200 F
250 - 300 F 1 hr.
E-XX27
150 - 200 F
150 - 200 F
250 - 300 F 1 hr.
E-60 or 7015
250 - 450 F
150 - 200 F
500 - 600 F 1 hr.
E-60 or 7016
250 - 450 F
150 - 200 F
500 - 600 F 1 hr.
E-7018
250 - 450 F
150 - 200 F
500 - 600 F 1 hr.
E-7028
250 - 450 F
150 - 200 F
500 - 600 F 1 hr.
E-80 or 9015
250 - 450 F
200 - 250 F
600 - 700 F 1 hr.
E-80 or 9016
250 - 450 F
200 - 250 F
600 - 700 F 1 hr.
E-80 or 9018
250 - 450 F
200 - 250 F
600 - 700 F 1 hr.
E-90 12015
250 - 450 F
200 - 250 F
650 - 750 F 1 hr.
E-90 12016
250 - 450 F
200 - 250 F
650 - 750 F 1 hr.
E-90 12018
250 - 450 F
200 - 250 F
650 - 750 F 1 hr.
E -XXX-15 or 16
250 - 450 F
150 - 200 F
450 F 1 hr.
Stainless
250 - 450 F
150 - 200 F
450 F 1 hr.
When being reconditioned, electrodes should not be baked for more than 4 hours and should be kept at temp for at least 30 minutes. Baking more than 3 times is not recommended.