of the electrodes listed below should be stored dry at room temp when in unopened
cartons.

Electrode
Classification
Recommended
Storage open Boxes
Holding
Oven
Reconditioning
E-XX10
Dry
@ room temp
Not
Recommended
Not
done
E-XX11
Dry
@ room temp
Not
Recommended
Not
done
E-XX12
Dry
@ room temp
Not
Recommended
Not
done
E-XX13
Dry
@ room temp
Not
Recommended
Not
done
E-XX14
150
– 200 F
150
– 200 F
250
– 300 F 1 hr.
E-XX20
150
– 200 F
150
– 200 F
250
– 300 F 1 hr.
E-XX24
150
– 200 F
150
– 200 F
250
– 300 F 1 hr.
E-XX27
150
– 200 F
150
– 200 F
250
– 300 F 1 hr.
E-60
or 7015
250
– 450 F
150
– 200 F
500
– 600 F 1 hr.
E-60
or 7016
250
– 450 F
150
– 200 F
500
– 600 F 1 hr.
E-7018
250
– 450 F
150
– 200 F
500
– 600 F 1 hr.
E-7028
250
– 450 F
150
– 200 F
500
– 600 F 1 hr.
E-80
or 9015
250
– 450 F
200
– 250 F
600
– 700 F 1 hr.
E-80
or 9016
250
– 450 F
200
– 250 F
600
– 700 F 1 hr.
E-80
or 9018
250
– 450 F
200
– 250 F
600
– 700 F 1 hr.
E-90
12015
250
– 450 F
200
– 250 F
650
– 750 F 1 hr.
E-90
12016
250
– 450 F
200
– 250 F
650
– 750 F 1 hr.
E-90
12018
250
– 450 F
200
– 250 F
650
– 750 F 1 hr.
E
-XXX-15 or 16
250
– 450 F
150
– 200 F
450
F 1 hr.
Stainless
250
– 450 F
150
– 200 F
450
F 1 hr.
When
being reconditioned, electrodes should not be baked for more than 4 hours and
should be kept at temp for at least 30 minutes. Baking more than 3 times is not
recommended.